Contact Us
HOME >Case Studies> SUGAR PLANTS

Rebuilding Of Pump Rotor

Industry Type
Sugar

Product Group
Electrode

OUR SOLUTION

Polarity
+VE

Power Source
Rectifier

Process
SMAW

Quantity (Kgs)
6

Current (amps)
98A

Size (mm)
3.15

Product
Lotherme-533

JOB PICTURES
Job Sketch With Dimension

Job Sketch With Dimension

ANALYSIS

Base Metal
Bronze

Previous Solution
Rebuild With Bronzoide-1(Esab Make)

Problem Due To
Abrasion

Type Of Problem
Frictional Wear

Component Name
Rotor

Equipment Name
Pump Rotor

1. Grind and remove the fatigue metal.

2. Clean the surface for welding

3. Weld the wear out area with loth-533, 3.15 mm.

4. Grind the surface upto level of surface.