HARDFACING OF PINCH ROLL

Industry Type

Product Group

ANALYSIS

BASE METAL
EN-9

PREVIOUS SOLUTION
ADORFONTECH make CITORIEL II

PROBLEM DUE TO
FRICTIONAL WEAR

TYPE OF PROBLEM
WEAR OUT

COMPONENT NAME
ROLLER

EQUIPMENT
PINCH ROLLER

JOB PICTURES

PHOTOGRAPH / JOB SKETCH

PHOTOGRAPH / JOB SKETCH

PHOTOGRAPH / JOB SKETCH

PHOTOGRAPH / JOB SKETCH

Our solution

Qty. (Kgs)
12

Current (AMPs)
70- 100

Size (mm)
4.00

Product
Lotherme 464

Qty. (Kgs)
10

Current (AMPs)
100-120

Size (mm)
4.00

Product
Lotherme 352

Procedure

1. Machine the uneven surface of roller to remove fatigue area & rust.

2. Build up upto 2.5mm thickness with Loth-352 to provide buffer layer.

3. Use Loth- 464 for the final surfacing.

4. Welding done successfully.

Further Reading on Case Studies

WELDING REBUILDING OF RING ROLLING CO-AXIAL ROLL

Read Case Study
Contact Us

Choose any option to contact us

", "search_title": null, "search_description": null, "category": "Pinch Roll"} ; $(document).ready(function () { $('.Industry_case_container .dropdown_case_study_2 .dropdown-item').on('click', function () { $('.custom-list-case-category span').html($(this).html()) }) $('.Industry_case_container .dropdown_case_study_3 .dropdown-item').on('click', function () { $('.mobile_mr_5 span').html($(this).html()) }) })