Industry Type
Product Group
ANALYSIS
DIMENSIONS (mm) T
25
COMP. WEIGHT (kgs)
650
BASE METAL
Spheroidal graphite Cast Iron
PREVIOUS SOLUTION
New Job Developed
PROBLEM DUE TO
High Pressure
TYPE OF PROBLEM
Joining of CI plate with casting
COMPONENT NAME
Cope Moulding Box
EQUIPMENT
High Pressure Moulding Box
JOB PICTURES
PHOTOGRAPH / JOB SKETCH WITH DIMENSION
Our solution
Qty.
25pc
Current (AMPs)
70- 100
Size (mm)
3.15
Product
D&H 1111-CI
Qty.
10pc
Current (AMPs)
70-85
Size (mm)
2.50
Product
Lotherme- 701
Procedure
1. Grind the entire area of welding to remove dust, sand and grease.
2. Prepare the V groove on Plate and Job.
3. Preheat the job and plate through Flame torch to remove the oil and grease soaked in job.
4. Start Weld with Loth-701 2.5mm single base layer.
5. Weld with 1111CI 3.15mm up to final layer.
Further Reading on Case Studies